Thermal cracks of implant-based zirconia four-unit restorations: A fractographic analysis of two restorations fractured during production.

J Prosthet Dent

Associate Professor, Department of Clinical Dentistry, Faculty of Medicine, University of Bergen, Bergen, Norway. Electronic address:

Published: September 2018

Two zirconia-based 4-unit restorations intended for the same patient fractured during the veneering process even though the prolonged cooling protocol recommended by the manufacturers was used. Fractographic analyses revealed that both restorations fractured as a result of thermal shock, but at different times during production. Further investigation is necessary to optimize the firing protocols for large zirconia-based restorations and avoid fracture due to thermal shock.

Download full-text PDF

Source
http://dx.doi.org/10.1016/j.prosdent.2017.11.018DOI Listing

Publication Analysis

Top Keywords

restorations fractured
8
thermal shock
8
restorations
5
thermal cracks
4
cracks implant-based
4
implant-based zirconia
4
zirconia four-unit
4
four-unit restorations
4
restorations fractographic
4
fractographic analysis
4

Similar Publications

Chapter 7: CLINICAL FORMS AT DIFFERENT AGES OF LIFE: CHILDHOOD, PREGNANCY, LACTATION, OLD AGE.

Ann Endocrinol (Paris)

January 2025

Université Paris-Saclay, Inserm, Endocrine Physiology and Physiopathology, Assistance Publique-Hôpitaux de Paris, Hôpital Bicêtre, Service d'Endocrinologie et des Maladies de la Reproduction and Centre de Référence des Maladies Rares de l'Hypophyse HYPO, F-94270 Le Kremlin-Bicêtre, France. Electronic address:

Primary hyperparathyroidism is rare in children. A germline mutation is identified in half of all children with primary hyperparathyroidism (70% of newborns and infants, and 40% of children and adolescents). The clinical manifestations of primary hyperparathyroidism in children are highly variable (often absent in newborns, rather severe and symptomatic in children and adolescents) and depend on the genetic cause, as well as the severity, rapidity of onset and duration of hypercalcemia.

View Article and Find Full Text PDF

Background: Aneurysmal bone cysts (ABCs) are benign, blood-filled neoplasms causing bone destruction, often requiring resection. However, challenges arise, especially at the cranio-cervical junction, where proximity to critical structures limits removal. Non-surgical options include selective arterial embolization (SAE) as main treatment, while Denosumab and centrifugated bone marrow emerge as experimental alternatives.

View Article and Find Full Text PDF

Corrective osteotomy for upper limb deformities caused by fractures, trauma, or degeneration necessitates detailed preoperative planning to ensure accurate anatomical alignment, restore limb length, and correct angular deformities. This review evaluates the effectiveness of a three-dimensional (3D) preoperative planning program and an image fusion system designed for intraoperative guidance during corrective osteotomy procedures. The application processes and clinical outcomes observed with these technologies in various surgical scenarios involving the upper extremities were summarized.

View Article and Find Full Text PDF

Patient: A 26-year-old man with localized tooth wear and demand for aesthetic rehabilitation of the anterior teeth presented to our department. The patient reported excessive consumption of energy drinks. Furthermore, multiple trauma and tooth fractures have occurred in the past.

View Article and Find Full Text PDF

Introduction: Traditional access cavity preparation involves removing the roof of the pulp chamber and smoothing the dentin bulges at the root canal orifice, thereby creating straight-line access. However, this may damage more healthy dental tissue and reduce the tooth's fracture resistance. This case series presents a novel minimally invasive endodontic protocol for one maxillary canine and four mandibular premolars, which required root canal therapy due to labial/buccal cervical decay that caused pulpitis or periapical periodontitis.

View Article and Find Full Text PDF

Want AI Summaries of new PubMed Abstracts delivered to your In-box?

Enter search terms and have AI summaries delivered each week - change queries or unsubscribe any time!