Aims: To evaluate the effect of the processing method (conventional sintering, S, and heat-pressing, HP) and addition of potassium titanate fibers, PTF, on the microstructure, mechanical properties (flexural strength, σf, and Weibull parameters, m and σ5%), slow crack growth parameters n (stress corrosion susceptibility coefficient), and optical properties (translucency parameter, TP, and opalescence index, OI) of a feldsphatic dental porcelain.
Methods: Disks (n = 240, Ø12 × 1 mm) of porcelain (Vintage-Halo, Shofu) were produced using S and HP methods with and without addition of 10 wt% (conventional sintering) or 5 wt% (heat-pressing) of PTF. For the S method, porcelain was sintered in a conventional furnace.